Q235NH耐候钢板材料

2023-02-28 18:09 浏览:1 来源:锅炉之家   
核心摘要:able data-draft-node="block" data-draft-type="table" data-size="normal" data-row-style="normal"YB /T 4112-2013牌号Q235NHL52350对应标准YB /T 4112-2013 结构用耐候焊接钢管 Welded steel tubes with atmospheric corrosion resistance for structur

able data-draft-node="block" data-draft-type="table" data-size="normal" data-row-style="normal">YB /T 4112-2013

牌号Q235NH
L52350
对应标准YB /T 4112-2013 结构用耐候焊接钢管 Welded steel tubes with atmospheric corrosion resistance for structural purposes
归类合金钢
说明此牌号化学成分(熔炼分析)应符合GB/T 4171的规定

牌号Q235NH
L52350
对应标准YB /T 4112-2013 结构用耐候焊接钢管 Welded steel tubes with atmospheric corrosion resistance for structural purposes
归类合金钢
说明此牌号化学成分(熔炼分析)应符合GB/T 4171的规定

牌号Q235NH
L52350
对应标准YB /T 4112-2013 结构用耐候焊接钢管 Welded steel tubes with atmospheric corrosion resistance for structural purposes
归类合金钢
说明此牌号化学成分(熔炼分析)应符合GB/T 4171的规定

Q235NH 化学元素成分含量(%)

成分C *SiMnPSCrNiCu
最小值-0.10.2--0.4-0.25
最大值0.130.40.60.030.030.80.650.55

* 供需双方协商,C的含量可以不大于0.15%。
① 为改善钢的性能,可以添加一种或一种以上的微量合金元素:Nb(0.015%~0.060%),V(0.02%~0.12%),Ti(0.02%~0.10%),Alt≥0.020%。若上述元素组合使用时,应至少保证其中一种元素含量达到上述化学成分的下限规定。
② 可以添加合金元素:Mo≤0.30%,Zr≤0.15%。
碳当量计算

Q235NH 机械性能

厚度tmm抗拉强度σb Mpa屈服点σs Mpa延伸率δ %
t≤16360~510≥235≥21
16<t≤40360~510≥225≥21
16<t≤40360~510≥215≥21